Texture analysis of ultra-high coercivity Sm2Co7 hot deformation magnets?

2021-05-06 08:55:38QiangMa馬強MeishuangJia賈美爽ZhifengHu胡智峰MingYue岳明YanliLiu劉艷麗TongyunZhao趙同云andBaogenShen沈保根
Chinese Physics B 2021年4期

Qiang Ma(馬強), Meishuang Jia(賈美爽), Zhifeng Hu(胡智峰), Ming Yue(岳明),Yanli Liu(劉艷麗),, Tongyun Zhao(趙同云), and Baogen Shen(沈保根),?

1State Key Laboratory of Magnetism,Institute of Physics,Chinese Academy of Sciences,Beijing 100190,China

2School of Science,Inner Mongolia University of Science and Technology,Baotou 014010,China

3College of Materials Science and Engineering,Beijing University of Technology,Beijing 100124,China

Keywords: Sm2Co7 magnet,spark plasma sintering,hot deformation,ultra-high coercivity,texture

1. Introduction

Sm–Co alloys such as SmCo5, Sm2Co17, and SmCo7have been extensively studied for high Curie temperature(TC)and large magnetocrystalline anisotropy(HA).[1–7]Sm2Co7is a kind of magnet with great potential for use in high temperature environment due to its large HA(>200 kOe)and good phase stability.[8–12]With the development of nanotechnology and the application of spark plasma sintering(SPS)technology in the field of nanocrystalline magnet preparation, the preparation of ultra-high coercivity(Hcj)Sm–Co bulk magnets becomes possible.[13]Preparation of Sm–Co alloy magnets by using SPS process can effectively avoid the abnormal growth of crystal grains and provide high coercivity.[14–16]Covercivity and phase stability of Sm2Co7type nanocrystalline magnets have been reported, but few studies have focused on the Sm2Co7anisotropic magnet.[17,18]Magnetic performance of isotropic nanocrystalline Sm2Co7is not high enough due to its low magnetic orientation.Hot deformation process is an effective method to obtain magnetic anisotropy of nanocrystalline magnets. However, strong c-axis crystallographic texture has never been reported so far for Sm2Co7nanocrystalline magnet. The present work is aimed to prepare Sm2Co7anisotropic magnet with strong texture by means of hot pressing and hot deformation,and to study the formation mechanism of the texture.

2. Experimental procedures

The Sm2Co7alloy ingots with a stoichiometric ratio 2:7(at.%) were prepared by induction melting of elemental Sm and Co both with 99.95% purity under the purified argon atmosphere. An excess of 5 wt.% Sm was used to compensate for its losses during the preparation.The ingots were quenched into ribbons at a wheel speed of 30 m/s and then high energy ball milled into amorphous powders. The powders were hot pressed (HP) at 700?C with a pressure of 450 MPa. In order to obtain anisotropic magnets, the isotropic hot pressed magnets were hot deformed (HD) with height reductions of 70%,80%,and 90%(named HD70%,HD80%,and HD90%,respectively)at the temperature of 720–750?C under the pressure of 20–50 kN. The magnetic properties of the samples were measured by vibrating sample magnetometer(VSM).Xray diffraction(XRD)measurement of the hot pressed and hot deformed samples has been performed by using Co Kα radiation. Electron backscatter diffraction (EBSD) was carried out to analyze the orientation and the mechanism of the texture formation. All of the test surfaces of the samples were perpendicular to the direction of pressure.

3. Results and discussion

As shown in Fig.1, the coercivity Hcjof the isotropic Sm2Co7HP magnet is 34.76 kOe, the remanence Mris 36.23 emu/g, and the maximum energy product (BH)maxis 3.76 MGOe. The sample of HD70% exhibits a coercivity as high as 50.68 kOe,which is the highest coercivity that SmCo bulk magnet has ever been reported to possess,and the remanence is 40.05 emu/g. As the die upset level increases to 80%,the coercivity of the magnet still remains 32.32 kOe, and the remanence increases to 48.56 emu/g. For the HD90% sample, the coercivity is drastically reduced to 4.60 kOe, while the remanence is increased to 63.10 emu/g and the maximum energy product is 8.21 MGOe. With the increase of height reduction, the increases of magnetic remanence and magnetic energy product arise from the enhancement of the magnetic anisotropy. The details of the magnetic properties of the Sm2Co7HP and HD magnets are shown in Table 1. The orientation degree of the magnet was calculated by the value of Mr/Ms(Msis the saturation magnetization at the magnetic field of 70 kOe). It is found that with the increase of the die upset level, the value of Mr/Msis increased from 82.20% to 94.74%, indicating that the orientation of c-axis of the magnets is optimized.[15]

The result of the Sm2Co7magnet HP sample analyzed using XRD is shown in Fig.2 by black line. As seen in the pattern,the magnet has a Sm2Co7single phase with a hexagonal Ce2Ni7-type structure(PDF#71-0387)at the room temperature. Figure 2 also shows the XRD patterns of the hotdeformed Sm2Co7magnets. As the die upset level increases,the peak of(00 12)is continually rising while the peak of(116)decreases, which means that the Sm2Co7grains have a preferred orientation during the HD process, resulting in a (00l)texture. The texture strength is quantitatively characterized by the value of I(0012)/I(116). The I(0012)/I(116)of the HP magnet is 0.53, then, with the amount of die upset level increased by 90%, the value of I(0012)/I(116)reaches 6.93, which is 13.08 times higher than that of HP magnet. The strong c-axis texture of the HD90%magnet is the reason for the high value of Mr/Msand high Mrin Table 1.

Fig.1. Hysteresis loop of the Sm2Co7 HP and HD magnets.

Fig.2. XRD patterns of the HP and HD Sm2Co7 magnets.

Table 1. Magnetic properties of the hot-pressed and hot-deformed Sm2Co7 magnets.

The magnets densities were tested using the Archimedes principle. As shown in Table 1, the density of the magnets after HD process is higher than that of the HP magnet,which indicates that some defects disappear in a long period of high temperature deformation during the HD process. As shown in Fig.3(a),the grain size of the HD 70%Sm2Co7magnet is about 300 nm,the grain boundaries are clearly visible,and the size of the grain is uniform,which are the reasons for obtaining ultra-high coercivity. In Fig.3(b),when the amount of the height reduction increases to 80%,the grains grow to 800 nm in size,which decreases the coercivity. The further growth of grains in the HD 90% samples results in the distribution of some micron-sized grains in the magnets,leading to the rapid decline of coercivity.

The orientation texture and microstructure of the HD Sm2Co7magnets were characterized by electron backscatter diffraction scanning (EBSD) analysis. Figures 3(d)–3(f) are EBSD-orientation imaging microscopy(OIM)scans,and figures 3(g)–3(i)are the corresponding inverse pole figures(IPFs)of the Sm2Co7magnets with deformations of the samples under HD70%,HD80%,and HD90%,respectively. In the OIMEBSD map, the color of a grain specifies its orientation according to the color code. As shown in Figs.3(d)–3(f), there are no unidentified regions in the OIM maps,indicating that all grains are Sm2Co7pure phase.As indicated by the color code,red represents that the grain orientation is parallel to the(001).Comparing the OIMs and their corresponding IPFs of different samples, it can be seen that the increase of deformation is beneficial to the formation of the (001) texture. When the height reduction is 90%, the pole density of the (001) direction is 9.02, which demonstrates that the magnet of HD 90%formed a strong (001) texture, providing a higher remanence for the magnet. Good agreement is obtained among the results of hysteresis loop,XRD,and EBSD.

Fig.3.(a)–(c)Grain size image quality(IQ)map,(d)–(f)OIM-EBSD scan,and(g)–(i)corresponding IPF of the hot deformed Sm2Co7magnets with 70%,80%,and 90%height reduction,respectively.

To analyze the distribution of the orientation angle of the HD magnets,the distribution of misorientation angles was calculated and illustrated in Fig.4. The black line in Fig.4 shows the angular distribution of the orientation difference in the random orientation,and the histograms show the angular distribution of the orientation difference measured by the specimens.The distribution of the grain misorientation angles of the HD magnet is different from the random distribution (black line in Fig.4), which is due to the continuous evolution of grain orientation during the deformation. The texture is strengthened with the increase of deformation degree, indicating that the concentration of grain misorientation angles is related to the texture. From Fig.4,it can be seen that the distribution of orientation difference of the HD90% magnet is concentrated around 30?,while the distribution of orientation difference of the HD70% and HD80% magnets is weaker at around 30?.This manifests that during the HD process, the grains tend to form a concentrated orientation relationship while forming the texture, and this orientation relationship is related to the mechanism of the texture formation of the grain rotation and recrystallization.[19–22]The results of XRD, EBSD, and misorientation analysis consistently show that the increase in deformation can promote the formation of (001) texture. Good(001)texture is primary for the permanent magnet materials to improve remanence.

Fig.4. Distribution of the grain misorientation angles of the Sm2Co7 HD magnets.

4. Conclusions and perspectives

In this study,anisotropic Sm2Co7magnets were prepared by using spark plasma sintering and hot deformation techniques.When the height reduction is 70%in the hot-deformed process, an ultra-high coercivity magnet with a coercivity of 50.68 kOe is obtained.The ultra-high coercivity is contributed to the uniform distribution of nano-scale grian size of HD70%samples. The Mr/Ms, XRD, and EBSD OIM analyses are in such a good agreement in proving that the hot deformation process can produce c-axis orientation texture of the Sm2Co7magnets, and the larger the deformation amount is, the better the c-axis texture of the magnets. And thus, the products of the Sm2Co7magnets are found acquired with higher remanence and magnetic energy. Future work will focus on the mechanism of texture evolution in Sm2Co7hot deformation magnets.

主站蜘蛛池模板: 最新亚洲人成无码网站欣赏网 | 91成人在线观看| 亚洲国产成人精品无码区性色| 67194亚洲无码| 国产精品亚洲一区二区三区z| 制服丝袜国产精品| 国产精品冒白浆免费视频| 99热这里都是国产精品| 狠狠色婷婷丁香综合久久韩国| 无码中文AⅤ在线观看| 九九九九热精品视频| 久久99国产综合精品1| av无码一区二区三区在线| 国内精品一区二区在线观看| 久久一本精品久久久ー99| 久久国产亚洲偷自| 五月婷婷丁香综合| 亚洲福利网址| 亚洲色图欧美视频| 无码高潮喷水在线观看| 久久人人爽人人爽人人片aV东京热| 国产免费网址| 91亚洲精选| 免费在线色| 欧美在线精品一区二区三区| 国内精品自在自线视频香蕉| 欧美日韩v| 国产精欧美一区二区三区| 久久国产精品嫖妓| 亚洲综合激情另类专区| 九九视频免费在线观看| 国产91高跟丝袜| 精品视频在线观看你懂的一区| 久久人午夜亚洲精品无码区| 亚洲日韩精品无码专区97| 国产欧美性爱网| 麻豆精品在线视频| 亚洲福利一区二区三区| 欧美日韩国产在线观看一区二区三区| 国产乱子伦手机在线| 在线观看亚洲成人| 国产精选自拍| 午夜成人在线视频| 黄色网站在线观看无码| 无套av在线| 亚洲av日韩av制服丝袜| 欧美一级在线| 玖玖精品在线| 91国内在线视频| 精品伊人久久大香线蕉网站| 国产福利小视频在线播放观看| 国产精品永久在线| 黑人巨大精品欧美一区二区区| 欧美在线黄| 日本久久网站| 99热亚洲精品6码| 国产精品视频第一专区| 特级欧美视频aaaaaa| 成人午夜福利视频| 国产免费观看av大片的网站| 曰韩人妻一区二区三区| 亚洲欧美一区二区三区图片| 欧美日韩中文国产| 麻豆精品久久久久久久99蜜桃| 四虎免费视频网站| 在线精品视频成人网| 制服丝袜一区二区三区在线| 制服丝袜国产精品| 在线免费不卡视频| 毛片久久网站小视频| 精品视频在线观看你懂的一区| 国产精品私拍99pans大尺度| 色男人的天堂久久综合| 在线观看欧美精品二区| 久久国产热| 亚洲欧美另类专区| 夜夜操天天摸| 国产噜噜噜视频在线观看| 九九九精品成人免费视频7| 成人免费黄色小视频| 成年女人a毛片免费视频| 日本a级免费|