Enhanced interface properties of diamond MOSFETs with Al2O3 gate dielectric deposited via ALD at a high temperature*

2021-05-24 02:23:44YuFu付裕RuiMinXu徐銳敏XinXinYu郁鑫鑫JianJunZhou周建軍YueChanKong孔月嬋TangShengChen陳堂勝BoYan延波YanRongLi李言榮ZhengQiangMa馬正強andYueHangXu徐躍杭
Chinese Physics B 2021年5期

Yu Fu(付裕), Rui-Min Xu(徐銳敏), Xin-Xin Yu(郁鑫鑫), Jian-Jun Zhou(周建軍),Yue-Chan Kong(孔月嬋), Tang-Sheng Chen(陳堂勝), Bo Yan(延波),Yan-Rong Li(李言榮),3, Zheng-Qiang Ma(馬正強), and Yue-Hang Xu(徐躍杭),?

1University of Electronic Science and Technology of China,Chengdu 611731,China

2Nanjing Electronic Devices Institute,Nanjing 210016,China

3Sichuan University,Chengdu 610041,China

4University of Wisconsin-Madison,Madison,WI 53705,USA

Keywords: diamond MOSFET,ALD temperature,pulsed I–V,interface trap,conductance method

1. Introduction

The ultra-wide band gap semiconductor diamond,due to its superior material properties, is considered to be a remarkable candidate for high-power and highfrequency applications.[1–3]Hydrogen-terminated (C–H) diamond, which has a negative electron affinity, forms a twodimensional hole gas (2DHG) surface channel regardless of how high the activation energy associated with p-type dopants is.[4]The conduction of the C–H diamond surface can be realized by exposing it to the air adsorbates or overcoating it with different oxides such as Al2O3and transition metal oxides (TMO). For these oxide materials, the empty electron states below diamond’s valence band maximum (VBM) capture the electrons in the diamond surface,which results in the upward band bending of VBM and the formation of the 2DHG layer.[2]Compared with high electron affinity insulators and other high-k oxides,[5]Al2O3forming by atomic layer deposition (ALD) is considered as a promising gate insulator and passivation layer for perusing high-performance C–H diamond MOSFETs.[6–9]Even so, the stability of device operation is still a critical limitation for the Al2O3-based C–H diamond FETs.[10]Theoretically, there are no surface states in a complete C–H diamond surface due to non-existence of dangling bonds. For this reason, there has not been made much effort devoted to the interface trap issues in C–H diamond.As a matter of fact, the gate dielectric Al2O3deposition condition can give rise to the traps at the interface. The trap-induced DCRF dispersion in diamond microwave device can restrict the available current and output power of diamond MOSFETs.[11]Interface traps have been investigated for diamond MOSFETs with ALD Al2O3deposited below 200°C.[12]However, the understanding of the Al2O3/C–H interface behavior for Al2O3deposited at even higher temperatures is still limited.

Since the C–H bonds and adsorbates generating holes are sensitive to factors such as environment and heat, the quality of the Al2O3films deposited at different temperatures[13]and their relevant transistor behaviors have been reported.[14]In fact, the bond enthalpy of C–H is higher than those of C–C and C–O,[15]which means that the C–H bond itself is quite stable. For the surface adsorbates, Al2O3deposited at 80°C proved to be an effective solution to preserve air adsorption.[8]However, it was shown that the adsorbate desorption occurs even at moderate temperatures(<200°C).[16]Notably,it was reported that a high-temperature(450°C)ALD process could also induce surface p-type conduction after the removal of air adsorbates, during which the surface holes were regenerated by the negative fixed charges in Al2O3.[7,9]But the thin 450-°C deposition Al2O3film is difficult to preserve new origins of hole accumulation,[17]it may limit the further development of the corresponding diamond MOSFETs in the high-frequency application, where high aspect-ratio is required.[18]Recently,the band offset of the 300-°C Al2O3depositing on C–H diamond claimed that this condition could also induce the p-type diamond conduction,[19]thus it is expected to achieve high output-current diamond devices using the thin 300-°C ALD grown Al2O3. Up to now, the significant interface properties of the C–H diamond MOSFETs with or without air adsorbates have not been unveiled. In this paper,we find that the fixed charges in Al2O3films are much lower than the 2DHG density. Our DC/pulsed I–V and frequency-dependent conductance measurements show that the interface trap states of the C–H diamond MOSFETs can be effectively suppressed at 300°C for ALD-Al2O3deposition in comparison with those deposited at 80°C, which indicates that the ALD deposition temperature is sufficiently high to achieve a high-quality interface for C–H diamond.

2. Device fabrication and characterization

The C–H diamond MOSFETs were fabricated on (100)-oriented type-IIa commercial diamond substrates. The substrates were prepared by using a strong acid solution(HNO3/H2SO4),and the purpose of this process is to remove the nondiamond phase.[1]The surface hydrogen-termination was realized by exposing the diamond surface to hydrogen plasma at 850°C for 20 min. Then, the samples were exposed to the air for a few hours to induce a high conductive 2DHG channel in the diamond surface. The gold(Au)metals were evaporated to protect the C–H diamond surface, afterwards, the metals covering the non-device areas were etched by using the potassium iodide (KI) solution. After exposing the diamond surface to the oxygen plasma,the device isolation was realized by replacing the C–H surface termination with the high resistive C–O surface termination.Drain and source electrode metals were formed by wet etching using KI solution.A 10-nm-thick (confirmed by the ellipsometry) Al2O3layer was coated on the C–H surface through the ALD method using Al(CH3)3and H2O as precursors. For one sample, the ALD deposition temperature was 80°C and for the other sample,it was 300°C.Aluminum(Al)gate metal was formed by using the thermal evaporation and lift-off process.The schematic diagrams of the fabrication processes are shown in Fig. 1. The gate width (WG) was 200 μm and the gate lengths (LG) were 0.1μm and 50μm,respectively.

Figure 2 shows the top-view SEM pictures of the 0.1-μm-LGdiamond devices. For the 0.1-μm LGdevices, DC and pulsed I–V curves were measured by using a Keithley 4200 semiconductor parameter analyzer. For the 50-μm LGFat-FET devices, besides the DC IGS–VGStest, capacitance and conductance measurements (ranging from 1 kHz to 1 MHz)were performed by using an Agilent B1500A semiconductor device analyzer. All measurements were conducted in a dark environment at room temperature(300 K).

Fig. 1. C–H diamond MOSFET fabrication processes. (a) Hydrogen-termination treatment, (b) deposition of Au to protect H-terminated diamond surface, and preparation of wet etching process of non-device areas, (c) device isolation by using oxygen plasma, (d) formation of source and drain electrodes,(e)ALD deposition of Al2O3 as gate insulator and passivation layer,and(f)gate fabrication and lift-off.

Figure 3(a) shows the measured C–VGcharacteristics of the gate–source capacitance of the Fat-FET devices at 1 MHz.The measured dielectric constants (ε) of Al2O3under 80-°C and 300-°C depositions are 8.75 and 6.78, respectively,which are consistent with the reported values.[20,21]The inset of Fig. 3(a) shows the calculated hole sheet density (np)versus gate voltage by integrating the C–VGcurve. The maximum 2DHG concentrations are 8.7×1012cm?2(300°C)and 1.1×1013cm?2(80°C), respectively. The inset shows that less channel holes exist in the 300°C-deposition diamond device than in the 80-°C case, which is possibly due to the fact that the conduction-related surface adsorbates of C–H diamond decrease with ALD deposition temperature increasing,which was indicated by the reported high-resolution transmission electron microscopy(HRTEM)images.[22]Furthermore,the Mott–Schottky plot is shown in Fig.3(b),from which the flat band voltage(VFB)was determined by linear extrapolation of the 1/C2–VGcurves to the abscissa.The background acceptor concentration (NA) extracted from the linear slope[23]are 1.1×1013cm?3and 2.2×1013cm?3for 80°C and 300°C,separately. The values suggest the high purity of the diamond samples. Taking into account the difference in work function between Al (4.3 eV) and C–H diamond (4.9 eV),[24]the theoretical flat band voltage (VFB0) was calculated to be 0.6 V.As indicated in Fig. 3(b), the measured VFBvalues for 80-°C and 300-°C depositions were 0.42 V and 0.74 V,respectively.According to Qox=Cox×(VFB?VFB0)/q, the fixed charges in the oxide layer(Qox)were estimated to be 8.7×1011cm?2(80°C) and ?5.9×1011cm?2(300°C). The negative fixed charges in the Al2O3deposited at 300°C could be due to some unoccupied levels in the bandgap of Al2O3located near the valence band edge of diamond.[25]The positive fixed charges observed in the 80-°C deposition device may be attributed to the oxygen vacancies in the oxide films.[26]

Fig.2. Topview SEM images of 0.1-μm LG:(a)80-°C deposition device and(b)300-°C deposition device.

The DC tests (ID?DC) show that both diamond devices’ maximum drain currents exceed ?400 mA/mm (LG=0.1μm), the IDS–VGScurve of the 80-°C and 300-°C deposition devices at VDS=?8 V are shown in Fig.4. Owing to the higher dielectric constant of the 80-°C deposition ALD Al2O3film,the device has exhibited better subthreshold performance.Pulsed I–V test is more effective than DC I–V measurement to characterize the traps-related performances because of its discontinuous signal excitation. Comparatively speaking, there is more severe current degradation in the 80-°C deposition diamond device when it is operated in the pulse I–V mode as shown in Fig. 5. Specifically, pulsed I–V (ID?pulse) measurements are employed to characterize the response of trap charging/discharging for the 0.1-μm-LGdiamond MOSFETs(VGSQ=5 V,VDSQ=?8 V).If the time constant of the charged traps is smaller than the pulse width, reduced holes and thus reduced current will be observed due to insufficient time for discharging from traps.[27]Figure 6 shows the ID?pulse/ID?DCcharacteristics measured at VGS=?2 V and VDS=?6 V.During the measurements, the pulse period used is 1 ms and the pulse width varies from 1μs to 100μs. For the 80-°C deposition device,a much more serious current degradation is observed, which suggests that it has more donor-like traps with a time constant smaller than 100 μs. In addition, it is worth noting that the drain current densities of the 300-°C deposition device in this work is the highest in the reported C–H diamond MOSFETs with 300-°C deposition ALD Al2O3.[14,19]

Fig. 3. (a) C–VG and (b) 1/C2–VG characteristics of the Al2O3/C–H diamond capacitor measured at 1 MHz and room temperature (RT). VFB of 0.42 V and 0.74 V are measured at 80-°C and 300-°C depositions, respectively,and VFB0 of 0.6 V is the theoretical value,it is fitting with the formula 1/C2=(?2/εε0eNA)(V ?VFB+kT/e).

Fig.4. DC IDS–VGS curve of 80-°C and 300-°C deposition 0.1-μm-LG devices at VDS=?8 V.

Fig.5. DC and pulsed I–V characteristics of(a)80-°C and(b)300-°C deposition diamond MOSFETs. In pulsed I–V case, quiescent bias point is selected at VGSQ=5 V,VDSQ=?8 V,and pulsed period and width are 1 ms and 1μs,respectively.

Fig.6. Ratio of pulse current to DC current(ID?pulse/ID?DC)characteristics of 80-°C and 300-°C deposition devices at VGS =?2 V and VDS =?6 V,with inset showing applied waveform during pulse I–V measurement.

3. The interface trap mapping by conductance method

In general, emission, rather than capture, is the rate limiting process.[28]Thus characterization of the trap emission time constant(τit)in diamond is crucial to the understanding of the interior trap behaviors. The frequency-dependent conductance method,proposed by Nicollian and Goetzberger,[28]is used to determine the interface traps behavior. The inset of Fig. 7 shows (a) the equivalent circuit of the measured MOS structure,where Cmand Gmdenote the measured capacitance and conductance, respectively; (b) the equivalent circuit of the MOS structure used for the conductance method,where Cit=qDitis the interface trap capacitance when Ditis given in eV?1·cm?2,Ritrepresents the energy loss caused by the capture-emission of carriers by interface trap, τit=RitCitis the interface trap time constant; (c) the simplified circuit with equivalent parallel conductance(Gp). In particular,series resistance (Rs) is introduced into the equivalent circuit considering high contact and access resistance of C–H diamond devices.[29]

Fig.7. Experimental data(circles)and fitting curves(lines)of Gp/ω ~ω.Plotted Gp/ω ~ω results of the 80-°C(left)and 300-°C deposition(right)devices are selected in their subthreshold bias regions. Inset shows(a)measured and[(b),(c)]equivalent circuits of MOS structure,correcting for series resistance(Rs)of contact resistance and access resistance of diamond FETs.

The Gp/ω ~ω characteristics at the selected voltages can be determined from Cmand Gm,[28]which can be expressed as

where Coxof 0.78 μF/cm2and 0.60 μF/cm2were extracted from the C–VGcharacteristics of the 80-°C and 300-°C deposition devices,respectively,

with ω =2π f being the radial frequency, Rsis the series resistance and determined from

Here,Gmaand Cmaare the measured conductance and capacitance in the accumulation mode. By assuming continuous interface trap levels,Gp/ω can be given by

where q is the elemental charge,and Ditdenotes the trap density. Mapping of Ditand τitcan be achieved by fitting the experimental Gp/ω ~ω data through using Eq.(5)as shown in Fig.7. For Eq.(5),the peak point(Gp/ω)maxis located at ωτit=2, and Ditcorrelated with (Gp/ω)maxequals (2.5/q)(Gp/ω)max. It can be seen that the measured conductance peaks of the 80-°C deposition device are broader than those predicted by Eq. (1), which was also observed in the nonannealed MOSFETs.[30]From Fig. 7, it can be seen that the 300-°C ALD process on the C–H diamond surface results in the suppression of the oxide charge non-uniformities and a higher interface quality. According to the Shockley–Read–Hall (SRH) statistic model,[28]the trap energy levels above diamond valence band(Eit–EV)can be deduced from the trap time constant(τit),which is written as

where vthis the thermal velocity,σpis the hole capture cross section, and NVis the effective density of states in diamond valence band. By assigning T =300 K, vth=1×107cm/s,σp=4×10?13cm?2,and NV=2.7×1019cm?3,figure 8(a)shows the mapping results of the trap density distributions and the corresponding energy levels, indicating that shallow traps(Eit?EV≈0.46 eV–0.56 eV)exist in diamond devices.Specifically,Ditin the 80-°C deposition device is in a range of 7.8×1013eV?1·cm?2–8.5×1013eV?1·cm?2for an energy level span of 0.46 eV–0.52 eV above the valence band of diamond. The higher trap density in the 80-°C deposition device is consistent with the results obtained from the above pulse I–V analysis. The devices with high interface traps may suffer the weak Fermi-level pinning (WFLP) effect, which will make the majority of charges in the MOS capacitor accommodated by interface traps, and cannot be found to operate as a classic MOS capacitor.[31]Notably,besides the depletion and accumulation performances in the C–V curves(Fig.3(a)),the typical current–voltage on/off characteristics (Fig. 4) can be observed for both devices. That is to say, the potential influence of the WFLP effect on our devices is generally acceptable. For the 300-°C deposition device, Ditis in a range of 2.2×1013eV?1·cm?2–5.1×1013eV?1·cm?2, with the energy level span of 0.53 eV–0.56 eV above the valence band of diamond. In fact, diamond material is expected to have deep energy level interface traps with long τit.[12]According to the SRH model,relation between the detectable trap energy range in the band gap of diamond (5.5 eV) and the correlated τitis shown in Fig.8(b). Notably,by using the conductance method at RT, only a small part of the trap states in diamond can be detected, and the calculated τitis around 1 year for the nearmidgap trap states even at 300°C(the grey line).

Fig.8. (a)Energy distributions of interface state density of Al2O3/C–H diamond structure,and(b)energy level Eit versus trap emission time constant τit in diamond band gap at RT(orange line)and 300 °C(grey line).

Figure 9 shows the schematic of energy band of the capturing process and emission process of the interface traps with different trap energy levels above the valence band of diamond (at the same gate voltage), and the red line and blue line demonstrate the energy band of the 80-°C and 300-°C deposition devices,respectively. Higher band up-bending of the 80-°C deposition suggests higher carrier concentration in the 2DHG channel, and it contains shallower energy level interface traps(ΔET)while the trap density is higher. As shown in Fig. 9(a), the interface traps capture the carriers when reducing VG. Figure 9(b)indicates that the filled interface traps with lower ΔETfirst emit the holes to the channel when increasing VG,while those interface traps with higher ΔETare more difficult to emit the holes. The gate leakage current characteristics of both Fat-FETs are shown in Fig.10,it can be noted that the IGSof the 80-°C deposition device begins to increase at the forward bias, while the 300-°C deposition device maintains low IGSin the total VGSrange. This can be attributed to the emission of the trapped holes into the gate electrode as suggested by the Frenkel–Poole (FP) emission effect,[14]since the detected interface trap of the 80-°C deposition device is higher than that of the 300-°C deposition device.

Fig.9. Schematic diagram of band diagrams of the capturing and emission processes of Al2O3/C–H diamond interface traps,where red and blue lines demonstrate the energy band of the 80-°C and 300-°C deposition devices,respectively. (a) Trap capturing with VG decreasing (hole accumulation),and(b)trap emission with VG increasing(hole depletion).

Fig.10. Gate leakage current of 50μm-LG diamond MOSFETs.

4. Conclusions and perspectives

In this paper,the comparative studies by using C–VGand pulse/DC I–V measurements are presented to characterize the traps-induced current degradation in the C–H diamond MOSFETs at different Al2O3deposition temperatures. The results show that while a wide range of ALD deposition temperatures can be used to fabricate diamond FETs with low gate leakage current and high drain current density, different trapped charges can exist in the Al2O3dielectric layer. Experimental results show that 300-°C ALD grown Al2O3can be a suitable gate dielectric and passivation layer solution for the prospective diamond power devices.

主站蜘蛛池模板: 黄色a一级视频| 内射人妻无码色AV天堂| 视频一本大道香蕉久在线播放| 日韩福利视频导航| 欧美三級片黃色三級片黃色1| 国产成人三级| 国产极品美女在线播放| A级全黄试看30分钟小视频| 人妻少妇乱子伦精品无码专区毛片| 国产人成网线在线播放va| 大乳丰满人妻中文字幕日本| 国产一区二区三区在线精品专区| 欧美精品成人一区二区视频一| 尤物国产在线| 久久99热这里只有精品免费看| 久久青青草原亚洲av无码| 国产精品国产三级国产专业不| 毛片最新网址| 浮力影院国产第一页| 欧美日本不卡| 久久精品无码专区免费| 国产真实自在自线免费精品| 国产精品自拍露脸视频| 人妻21p大胆| 亚洲午夜片| 在线视频亚洲欧美| 国产成人8x视频一区二区| 制服丝袜国产精品| 亚洲天堂.com| 国产成人综合亚洲欧美在| 国产www网站| 啊嗯不日本网站| 久久综合九九亚洲一区| 国产精品不卡片视频免费观看| 热这里只有精品国产热门精品| 亚洲日本韩在线观看| 中文国产成人久久精品小说| 香蕉精品在线| 亚洲中文字幕在线精品一区| 国产网站黄| 国产高清在线精品一区二区三区| 国产爽妇精品| 最新无码专区超级碰碰碰| 亚洲国产高清精品线久久| 国产中文在线亚洲精品官网| 在线观看的黄网| 国产一区二区三区在线观看视频 | 亚洲成肉网| 香蕉eeww99国产在线观看| 亚洲国内精品自在自线官| 精品撒尿视频一区二区三区| 午夜国产小视频| 国产无码精品在线播放| 日韩av无码DVD| 久久semm亚洲国产| 国产午夜精品一区二区三| 色综合天天综合中文网| 日本成人在线不卡视频| 99热这里只有精品国产99| 免费观看男人免费桶女人视频| 精品国产中文一级毛片在线看| 国产精品人人做人人爽人人添| 亚洲男人天堂网址| 欧美精品伊人久久| 欧美精品一二三区| 欧美啪啪网| 蜜臀AV在线播放| 国产成人综合欧美精品久久| 亚洲制服中文字幕一区二区| 中文字幕天无码久久精品视频免费 | 欧美成人h精品网站| 99久视频| 久久精品人人做人人| 久草视频一区| www.狠狠| 成年女人a毛片免费视频| 怡春院欧美一区二区三区免费| 欧美在线一二区| 久久久久人妻一区精品色奶水| 国产精品视频免费网站| 精品第一国产综合精品Aⅴ| 亚洲色无码专线精品观看|