Perpendicular magnetic anisotropy of Pd/Co2MnSi/NiFe2O4/Pd multilayers on F-mica substrates

2022-01-23 06:35:30QingwangBai白青旺BinGuo郭斌QinYin尹欽andShuyunWang王書運
Chinese Physics B 2022年1期

Qingwang Bai(白青旺), Bin Guo(郭斌), Qin Yin(尹欽), and Shuyun Wang(王書運)

School of Physics and Electronics,Shandong Normal University,Ji’nan 250358,China

Keywords: perpendicular magnetic anisotropy,Co2MnSi,ferrimagnetics NiFe2O4

1. Introduction

Magnetic tunneling junctions (MTJs) with perpendicular magnetic anisotropy (PMA) have high enough thermal stability and low critical switching current in magnetoresistive random access memory (MRAM), so magnetic recording materials with PMA have become one of the research hot spots in recent years.[1-3]Over the years,Co-based multilayer films(Co/Pd and Co/Pt),rare-earth and transition metal alloys(GdFeCo) and L1 ordered alloys (CoPt and FePt) have been studied in depth.[4-6]However, these materials have some limitations such as inadequate chemical or thermal stability and low spin polarizability.[7,8]Full Hessler alloy Co2MnSi(CMS) has a series of advantages, such as good thermal stability, nearly 100% spin polarizability, high Curie temperatureTc(~1000 K), very low Gilbert damping constantα(~0.001), and large tunneling magnetoresistance(TMR).So it has attracted widespread attention from people in recent years.[9,10]CMS is a promising candidate material for magnetic recording.[11-13]

Studies have shown that strong PMA can be induced by the interface effect between ferromagnetic metals (FM)and metal oxides (OX), such as CoFeB/MgO, Co/MgO, and Co2MnSi/NiO structures.[14-16]Moreover,spinel oxides,such as MgAl2O4and MgGa2O4, can further improve the performance of MTJs when used as a tunnel barrier due to their small lattice mismatch with typical FM electrodes.[17,18]NiFe2O4(NFO)is a typical ferromagnetic spinel oxide with high magnetic ordering temperature and high saturation susceptibility. It is a very attractive candidate material for spintronic devices.[19]In particular, NFO has been successfully used as a spin-filtering tunnel barrier with a spin filtering efficiency of up to 22% at low temperatures.[20]Therefore, using NFO as a tunneling barrier for MTJs will increase the electron polarizability and thus increase TMR. Liet al.predicted by theoretical calculation that NFO could induce large PMA.[21]So far, there have been few studies on the PMA of CMS/NFO heterostructures.

In addition, mica substrate has a flat and inert surface, which is very conducive to the epitaxial growth of two-dimensional materials.In recent years, many researchers have grown high-quality thin film materials on mica substrates.[22-24]However, in the field of magnetic thin film materials, there are few studies on preparing of samples on mica substrates. In this paper, the magnetic properties of Pd/CMS/NFO/Pd multilayers deposited on mica substrates by sputtering were compared with those deposited on glass substrates and Si/SiO2substrates.

2. Experiments

All samples in this experiment were deposited on fluorphlogopite mica (F-mica) substrates at 350°C by magnetron sputtering unless otherwise specified. The background vacuum before deposition is better than 6×10-4Pa. The substrate is rotated at 15 rpm to ensure the uniformity of sputtering deposition. The structure and preparation details of this series of samples are shown in Table 1 (symbols or numbers in parentheses indicate film thickness in nanometers). In this experiment,all NFO layers prepared by sputtering were soon exposed to an oxygen atmosphere of 0.5 Pa for 5 min unless otherwise stated. In this paper,the sputtering rate of each target material is measured by mass weighing method, and the required thickness of film is obtained by controlling the sputtering time. The sputtering parameters of all the targets are shown in Table 2.

The magnetic properties of the samples were measured by an alternating gradient magnetometer AGM:MicroMag 2900.The Hall curve of the samples was measured by four-probe method. The surface morphology of different substrates was measured by atomic force microscopy AFM:BY-5000.

Table 1. Series of samples and corresponding experimental variables.

Table 2. Sputtering parameters for all targets.

3. Results and discussion

3.1. Effects of the thickness of CMS layer on PMA

Figure 1(a) shows the Hall loops of a series of Pd(3)/CMS(tCMS)/NFO(0.8)/Pd(3) multilayers with different CMS thicknesses. Figure 1(b)shows the coercivity field(HC)and Hall resistance(RHall)as functions of the thickness of the CMS layer. WhentCMS=3 nm,the films do not exhibit PMA,because the relatively thin CMS layer cannot form strong interface effect with Pd and NFO to overcome the demagnetization energy.[25]The squareness of Hall loops becomes better andRHallincreases with the increase of CMS thickness. The close to 1 of squareness and largeRHallwere observed at thetCMS=5 nm,indicating that the sample has a strong PMA.As the thickness of CMS continues to increase,the demagnetization energy of the sample increases,so that theRHalldecreases gradually. WhentCMS=9 nm, the PMA is disappear, which is attributed to the interfacial anisotropy energy cannot overcome the demagnetization energy.[15,16]HCof the samples decreases slightly with the increase of CMS thickness,which can be found in Fig.1(b).

Figure 1(c)show the in-plane and out-of-plane hysteresis loops of Pd(3)/CMS(5)/NFO(0.8)/Pd(3).A typical square outof-plane hysteresis loop is observed, with 100% remanence,and a coercive field of about 425.36 Oe(1 Oe=79.5775 A/m).These data are basically consistent with those of Hall loops.The magnetic anisotropy energy density (Keff) value can be estimated from the area difference between the magnetization curve of the in-plane and that of out-of-plane:Keff=∫[M⊥-M‖]dH, whereM⊥is the out-of-plane magnetization,M‖is the in-plane magnetization. The sampleKeffvalue of 0.6711 Merg/cm3was calculated, reflecting the excellent PMA performance of the sample.[14]

Fig.1. (a)Hall loops of Pd(3)/CMS(tCMS)/NFO(0.8)/Pd(3)under different tCMS,(b)tCMS dependencies of RHall (black)and HC (blue),(c)in-plane and out-of-plane hysteresis loops of Pd(3)/CMS(5)/NFO(0.8)/Pd(3).

3.2. Effect of NFO thickness on PMA

Hall loops of a series of Pd(3)/CMS(5)/NFO(tNFO)/Pd(3)multilayers with different NFO thicknesses are shown in Fig. 2(a).In general, the PMA of FM/OX multilayers is strongly affected by the degree of oxidation at the interface.[26,27]The thickness of the oxide layer is a key factor affecting the oxidation state of the interface, so appropriate oxide layer thickness is crucial for obtaining strong PMA.[14-16,28]WhentNFO=0.2 nm or 1.4 nm,the CMS/NFO interface was in the state of under-oxidation and overoxidation, respectively, the sample is displayed in-plane magnetic easy axis. WhentNFO=0.8 nm,the sample has excellent Hall loops squareness and largeRHall,which reflects the sample has strong PMA. ThetNFOdependence ofHCandRHallwere basically consistent as observed in Fig.2(b),suggesting that theHCof the sample with strong PMA was relatively large only under the change oftNFO. Similar phenomena have been observed in CMS/MgO, CMS/MAO and other structures.[28,29]In conclusion, when the thickness of NFO layer was 0.8 nm,the optimal interfacial oxidation degree of FM/OX interface was obtained,and PMA of the sample is the strongest.

Fig.2. (a)Hall loops for Pd(3)/CMS(5)/NFO(tNFO)/Pd(3)with various tNFO from 0.2 nm to 1.4 nm,(b)RHall (black)and HC (blue)dependence on tNFO.

3.3. Effect of TO2 on PMA

It is well known that PMA is mainly originated from the orbital hybridization of Co-3d and O-2p at the interface of CMS/OX multilayers.[29,30]During the preparation of oxide layer, a certain proportion of O2is usually injected into the sputtering gas in order to reduce oxygen loss and oxygen vacancy in the oxide layer.[14-16]However,the ferromagnetic layer will be overoxidized if too much oxygen is introduced. Therefore, in this experiment, the oxide layer was sputtered in high purity Ar environment,and then exposed to high purity O2atmosphere, so that the sputtered oxide layer was sufficient oxidized to eliminate oxygen loss and oxygen vacancy. Figure 3(a) shows the Hall loops of a series of Pd(3)/CMS(5)/NFO(0.8)/Pd(3)multilayers with differentTO2(exposure time to oxygen atmosphere after sputtering NFO layer). Figure 3(b) shows theRHallandHCdependence ofTO2. WhenTO2=0 min,the Hall loops squareness is poor andRHallis small,indicating that the PMA of the sample is weak.This is because the oxygen loss and the oxygen vacancy in the NFO lead to insufficient Co-O orbital hybridization at the CMS/NFO interface,which resulting in a weak interface effect of CMS/NFO.[17,31]The close to 1 of squareness and largeRHallcan be observed at theTO2≥5 min, showing that the sample exhibited strong PMA. TheRHallandHCof the sample remain basically unchanged asTO2continues to increase.To sum up, oxygen loss and oxygen vacancy in NFO can be basically eliminated atTO2≥5 min,and no overoxidation will occur at the CMS/NOF interface.

Fig. 3. (a) Hall loops for Pd(3)/CMS(5)/NFO(0.8)/Pd(3) with various TO2 from 0 min to 30 min,(b)RHall (black)and HC (blue)dependence on TO2.

3.4. Effect of substrates on PMA

The Hall loops and the in-plane and the out-of-plane hysteresis loops of a series of Pd(3)/CMS(5)/NFO(0.8)/Pd(3)multilayers deposited on different substrates are shown in Fig. 4. The samples deposited on F-mica substrates have largerRHallandHCcompared with those deposited on glass and Si/SiO2substrates. SuitableHCcan make the magnetic properties of thin films more stable and facilitate the miniaturization of devices.[32]By calculating theKeffvalue of these samples, it was found that theKeffvalue of the sample deposited on the F-mica substrate is 0.6711 Merg/cm3, which was about 30% larger than that of the samples deposited on the glass (0.475 Merg/cm3) and Si/SiO2(0.511 Merg/cm3)substrate. The surface morphologies of three different substrates were observed by AFM, as shown in Fig. 5. As can be seen from the figure, F-mica substrate has a flatter surface than glass and Si/SiO2substrate. The roughness of F-mica substrate is 0.083 nm,which is only one third of that of glass substrate (0.231 nm) or Si/SiO2substrate (0.243 nm). The flatness of the substrate provides conditions for the deposition of high quality films and interfaces on it, which is more conducive to improving the PMA of multilayers.[22-24,33]

Fig. 4. (a) Hall loops and (b)-(d) in-plane and out-plane M-H loops of Pd(3)/CMS(5)/NFO(0.8)/Pd(3) multilayers deposited on different substrates.

Fig.5. Surface morphologies of(a)F-mica substrates,(b)glass substrates,and(c)Si/SiO2 substrates.

4. Conclusion

A series of Pd(3)/CMS(tCMS)/NFO(tNFO)/Pd(3)multilayers were fabricated on F-mica substrates by magnetron sputtering. The Pd(3)/CMS(5)/NFO(0.8)/Pd(3) multilayer structure with the best PMA performance was obtained by adjusting the thickness of CMS and NFO,and the sampleKeffvalue was 0.6711 Merg/cm3. In this study,the NFO layer fabricated by sputtering in high purity Ar environment was exposed to high purity O2atmosphere for 5 min,which could effectively eliminate the oxygen loss and oxygen vacancy in NFO,ensuring enough Co-O orbital hybridization at the CMS/NFO interface, and thus effectively improve the sample PMA. Compared with the samples deposited on glass and Si/SiO2substrates, the multilayers deposited on F-mica substrates have largerRHallandHC,and theKeffvalue is also significantly increased. TheKeffvalue of the Pd/CMS/NFO/Pd multilayers deposited on the F-mica substrate is 0.6711 Merg/cm3,which is about 30%larger than that of the samples deposited on the glass (0.475 Merg/cm3) and Si/SiO2(0.511 Merg/cm3) substrates. In the following work,we will try to applying a magnetic field during the film deposition to continue to enhance the PMA of the multilayers.[34]

Acknowledgment

Project supported by the Shandong Provincial Natural Science Foundation,China(Grant No.ZR2018MEM004).

主站蜘蛛池模板: 久久毛片基地| 久久久黄色片| 精品一区二区三区四区五区| 欧美影院久久| A级全黄试看30分钟小视频| 亚洲愉拍一区二区精品| 亚洲中文精品久久久久久不卡| 国产福利影院在线观看| 久久久久国产精品免费免费不卡| 国产精品一区二区久久精品无码| 国产对白刺激真实精品91| 啦啦啦网站在线观看a毛片| 欧美日韩一区二区在线免费观看 | 日韩国产亚洲一区二区在线观看| 亚洲天堂2014| 亚洲黄色网站视频| 亚洲精品国产首次亮相| 国产一级在线观看www色| 麻豆精品在线视频| 亚洲欧洲日本在线| 福利小视频在线播放| 国产精品亚洲一区二区三区z| 精品综合久久久久久97超人| 日韩大乳视频中文字幕 | av在线无码浏览| 日本人妻一区二区三区不卡影院 | 2021国产乱人伦在线播放| 大陆国产精品视频| 国产综合欧美| 99爱视频精品免视看| 99热这里只有精品免费国产| 亚洲欧美一级一级a| 久久久久久久久久国产精品| 人与鲁专区| 久久精品欧美一区二区| 人妻中文久热无码丝袜| 免费看一级毛片波多结衣| 久久久久夜色精品波多野结衣| 色九九视频| 国产成人调教在线视频| 久久永久精品免费视频| 欧美日韩北条麻妃一区二区| 亚洲高清在线天堂精品| 色老二精品视频在线观看| 成人在线综合| 久久综合伊人77777| 无码人妻免费| 欧美日韩精品一区二区在线线 | 精品视频在线观看你懂的一区| 久久香蕉国产线| 精品国产成人a在线观看| 国产精品永久不卡免费视频| 波多野结衣一区二区三区AV| 久久人体视频| 中文字幕2区| 国产在线观看精品| 国产高清免费午夜在线视频| 国产亚洲欧美在线中文bt天堂 | 77777亚洲午夜久久多人| 9cao视频精品| 国产精品夜夜嗨视频免费视频| 亚洲一区二区日韩欧美gif| 2018日日摸夜夜添狠狠躁| 国产丝袜啪啪| 久久综合久久鬼| 日韩人妻无码制服丝袜视频| 四虎国产永久在线观看| 免费全部高H视频无码无遮掩| 国产精品免费电影| 日韩专区欧美| 国产在线观看一区二区三区| 婷婷开心中文字幕| 国产91蝌蚪窝| 欧美国产日韩在线播放| 精品色综合| 成人福利一区二区视频在线| 成年人午夜免费视频| 国产高清在线观看| 亚洲无码高清免费视频亚洲| 色综合天天综合| 国产无人区一区二区三区| 免费女人18毛片a级毛片视频|