999精品在线视频,手机成人午夜在线视频,久久不卡国产精品无码,中日无码在线观看,成人av手机在线观看,日韩精品亚洲一区中文字幕,亚洲av无码人妻,四虎国产在线观看 ?

A polarization mismatched p-GaN/p-Al0.25Ga0.75N/p-GaN structure to improve the hole injection for GaN based micro-LED with secondary etched mesa

2023-02-20 13:16:58YidanZhang張一丹ChunshuangChu楚春雙ShengHang杭升YonghuiZhang張勇輝QuanZheng鄭權QingLi李青WengangBi畢文剛andZihuiZhang張紫輝
Chinese Physics B 2023年1期

Yidan Zhang(張一丹), Chunshuang Chu(楚春雙), Sheng Hang(杭升), Yonghui Zhang(張勇輝),Quan Zheng(鄭權), Qing Li(李青), Wengang Bi(畢文剛), and Zihui Zhang(張紫輝),?

1State Key Laboratory of Reliability and Intelligence of Electrical Equipment,Hebei University of Technology,Tianjin 300401,China

2School of Electronics and Information Engineering,Hebei University of Technology,Key Laboratory of Electronic Materials and Devices of Tianjin,Tianjin 300401,China

3School of Electrical Engineering,Hebei University of Technology,Tianjin 300401,China.

4State Key Engineering Center of Flat-Panel-Display Glass and Equipment,Shijiazhuang 050035,China

Keywords: μLED,polarization mismatch,secondary etched mesa,hole injection

1. Introduction

When compared with organic light-emitting diodes(LEDs),III-nitride based LEDs have advantages of low power consumption, long operation life-time, high luminous efficiency, quick response, etc.[1–3]Meanwhile, improved light extraction efficiency (LEE), better current spreading and enhanced heat dissipation can be further achieved by reducing the LED chip size,modifying the inclined sidewall angle and so on.[4–6]Thus, the micro-light emitting diodes (μLEDs)are considered as promising candidates in applications of implantable optoelectronic equipment, display, optical communication, biomedical detection, etc.[7]However, as the size of the LED chip becomes smaller, the external quantum efficiency(EQE)and the optical power decrease significantly,[8,9]which is due to the sidewall damages on the mesa. These surface damages are caused by the plasma-assisted dry etching process. They form carrier leakage channels and produce nonradiative recombination.[10,11]In order to reduce the influence of the defected region on the optoelectronic properties for GaN-based μLEDs, the surface and sidewall defects for μLEDs can be repaired by optimizing the chip fabrication process. For example, the defects on mesa sidewalls can be reduced by optimizing the annealing time and using chemical treatment.[12,13]Moreover,an insulation passivation layer,e.g., SiO2deposited by plasma-enhanced chemical vapor deposition(PECVD)or atomic layer deposition(ALD)systems,can also annihilate surface defects for μLEDs.[14,15]According to our recent report,a resistive ITO/p-GaN junction at the mesa edge for GaN-based μLEDs can function as a current blocking layer,and as a result,the holes can be kept apart from the mesa edge.[16]The current leakage and the surface recombination can be further decreased if one can both make a more resistive junction and generate the energy barriers simultaneously at the mesa periphery. For that goal,our group proposed an ITO/Ta2O5/p-GaN periphery junction at the μLED mesa edge.[17]The most significant advantage of this design is that the large relative dielectric constant of 26 for the Ta2O5layer can generate energy barriers in the p-GaN layer,and this helps to confine the holes in the central region for the μLED mesa.According to the report by Kouet al.,[10]the hole injection can be promoted when the surface recombination can be significantly suppressed. Nevertheless, there is little possibility of completely eliminating the hole diffusion to the mesa edge.Hence, it becomes increasingly important that the hole injection efficiency shall be enhanced for GaN-based μLEDs.

In this work, we design and fabricate a GaNbased μLED with a p-GaN/p-Al0.25Ga0.75N/p-GaN structure.Such p-GaN/p-Al0.25Ga0.75N/p-GaN structure can generate polarization-induced electric field that can help to make“hot”holes. In addition,a secondary etched mesa is also fabricated and passivated by using SiO2insulating layer.By doing so,the current can be effectively confined in the non-defected area,which suppresses the nonradiative recombination in the mesa edge. As a result,the hole injection can be improved while the surface nonradiative recombination can be decreased. This in turn improves the EQE and reduces the leakage current for the proposed μLED.

2. Structure design and parameters

In order to show the effectiveness of the proposed GaNbased μLED on the improvement for the optoelectronic characteristics, the epitaxial wafers for GaN-based μLEDs are grown on [0001]-oriented sapphire substrate by using metalorganic chemical vapor deposition (MOCVD) system. Both μLED wafers have a 2 μm thick GaN layer with the electron concentration of 5×1018cm-3. After that, 5 pairs of In0.15Ga0.85N/GaN multiple quantum wells (MQWs) are grown to produce the peak emission wavelength of~450 nm.The thicknesses of the quantum wells and the quantum barriers are~3 nm and~12 nm, respectively. Then, a 25 nm thick p-Al0.25Ga0.75N electron blocking layer (p-EBL) with the hole concentration of 3×1017cm-3is utilized to reduce the electron leakage from MQWs. Next, an 80 nm thick p-GaN layer and a 10 nm thick p+-GaN layer serve as the hole injection layer for the reference μLED wafer, for which the hole concentrations are estimated to be 3×1017cm-3and 1×1021cm-3, respectively. Nevertheless, different from the reference μLED wafer, the proposed μLED wafer has a 3 nm thick p-Al0.25Ga0.75N layer with the hole concentration of 3×1017cm-3inserted into the p-GaN layer, so that a 30 nm p-GaN/3 nm p-Al0.25Ga0.75N/50 nm p-GaN structure can be formed. Different μLEDs have been fabricated such that devices A and B are made of the reference and the proposed μLED wafers in Figs. 1(a) and 1(b), respectively. The scanning electron microscope(SEM)image for the fabricated μLED is shown in Fig.1(c). Details regarding the chip fabrication processes will be presented subsequently.We have conducted the cross-sectional transmission electron microscope(TEM) measurement in the p-type region for devices A and B that are presented in Figs. 1(d) and 1(e), respectively. We can see that the p+-GaN layer,the p-GaN layer and the p-EBL are grown as the pre-set thickness for device A.Moreover,the thin p-Al0.25Ga0.75N layer with the thickness of~3 nm has also been inserted into the p-GaN layer during the epitaxial growth process.

Fig.1. Schematic diagrams for (a) device A and (b) device B with the p-GaN/p-Al0.25Ga0.75N/p-GaN structure and secondary etched mesa.(c)SEM image for the fabricated μLED with the chip size of 40×40 μm2. Cross-sectional TEM images of the p-type region for(d)device A and(e)device B.

The fabrication processes for the two μLEDs are as follows. Firstly,for both devices,a square mesa is patterned and dry etched by using the inductively coupled plasma(ICP)system to expose the n-GaN layer. The mesa size is 40×40 μm2and the mesa height is 500 nm. Then,the secondary mesa for device B is etched on both sides of the p-type region. The height and the width for the secondary mesa are~60 nm and~30 μm, respectively. For both devices, the SiO2insulating layer of~200 nm is deposited on the mesa sidewalls by using PECVD system, which is used to passivate the sidewalls defects and isolate the contact between the p-electrode and the n-GaN layer. After patterning the SiO2insulating layer so that the metal contact regions can be exposed, a thin Ni/Au(10 nm/10 nm) is deposited on the p+-GaN layer serving as the current spreading layer. The Ni/Au is annealed in the oxygen environment at the temperature of 450°C for 3 min to form the ohmic contact.[18]On the top of the Ni/Au current spreading layer, we deposit Ni/Au (10 nm/200 nm) so that the Ni/Au/Ni/Au p-type electrode is formed. Next, the Ti/Al/Ti/Au(20 nm/30 nm/60 nm/100 nm)is deposited on the n-GaN layer as the n-type ohmic contact.

The two μLEDs are numerically investigated by using APSYS software so that an in-depth understanding such as carrier transport and recombination processes can be obtained. The physical equations including Poisson’s equation,Schr¨odinger equation, drift-diffusion equation, etc. are selfconsistently solved.[19]The Shockley–Read–Hall (SRH) recombination lifetime is set to 100 ns and the Auger recombination coefficient is 1×10-30cm6/s in our model for the nonradiative recombination process.[20]The band offset ratio between the conduction band and valence band is set to 0.7/0.3 for the InGaN/GaN MQWs.[10]The LEE for the studied blue μLEDs is set to 60% by compromising our measured EQE and the reported value.[21]Additionally, we also set the defect model in our simulations. The electron trap level is set at 0.24 eV below the conduction band (i.e.,Ec-0.24 eV),for which the trap density and the capture cross section are 1×1013cm-3and 3.4×10-17cm2, respectively.[10,22]The hole trap level is set at 0.46 eV above the valence band(i.e.,Ev+0.46 eV), for which the trap density and the capture cross section are 1.6×1013cm-3and 2.1×10-15cm2,respectively.[10,23]Other important parameters in our simulation model can also be found in Ref.[24].

3. Results and discussion

By using a calibrated integrating sphere, we show the measured electroluminescence (EL) spectra in terms of various injection current densities for devices A and B in Figs.2(a)and 2(b), respectively. Note, the measured devices are not packaged with bare μLED dies, so that only part of the photons can be collected by our optical fiber. It shows that the EL intensity for devices A and B increases as the current density increases from 50 A/cm2to 200 A/cm2. Meanwhile, the EL intensity for device B is always stronger than that for device A at the same current density level. The inset in Fig.2(a)shows the illuminating device taken under the optical microscope system. The blue emission with the peak wavelength of~445 nm can be observed,which agrees with the set InN composition in the MQWs.

Fig.2. Measured EL spectra for (a) device A and (b) device B at varying injection current density levels. The inset in (a) shows the image for the illuminating μLED at the current density of 200 A/cm2.

Fig.3.(a)Measured and(b)calculated EQE and optical power density as a function of the injection current density for devices A and B,respectively.

In order to better understand the impact of the proposed p-GaN/p-Al0.25Ga0.75N/p-GaN structure and the secondary etched mesa of the p-type region,we then experimentally and numerically obtain the EQE and optical power density at various injection current density levels for devices A and B in Figs. 3(a) and 3(b), respectively. We can see that the measured EQE and optical power density for device B are both higher than those for device A, which is consistent with the trend of the calculated results in Fig.3(b). This also indicates the reliability of our simulation model. The results presented in Fig. 3(a) are also consistent with the EL profiles in Fig. 2.At the current density of 200 A/cm2, the measured efficiency droop levels are 65.2% and 43.8% for devices A and B, respectively according to Fig.3(a). These values are 23.7%and 15.6%for devices A and B,respectively according to the numerical results in Fig.3(b). The reduced efficiency droop obtained both experimentally and numerically for device B can be well attributed to the increased hole injection.[25]

In order to reveal the underlying physical mechanism for the enhanced EQE and optical power for device B, we calculate the electric field and the hole concentration profiles for devices A and B in Figs. 4(a)–4(c), respectively. Figure 4(a) shows that the polarization electric field is formed at the multiple heterojunction interfaces for the p-GaN/p-Al0.25Ga0.75N/p-GaN structure. We define that the positive electric field is along the [0001] orientation. When we look into the electric field profile in the thin p-Al0.25Ga0.75N layer,we can infer that the holes may lose energy as they travel through the thin p-Al0.25Ga0.75N layer. To better investigate the net energy (W) that the holes obtain from the p-type region for devices A and B,we integrate the electric field by following the equationW=eEfield·dx,in whicheis electron charge,Efielddenotes the electric field profile andlrepresents the integration range. The values ofWobtained by the holes are-0.09 eV and-0.18 eV for devices A and B at the current density of 200 A/cm2, respectively. The negative value ofWmeans that the holes obtain the energy from the p-type region and become “hot”. Therefore, the injection of holes into the MQWs can be effectively promoted and the radiative recombination in the whole active region can be improved for device B according to Fig. 4(b). Figure 4(c) presents the lateral hole concentration distribution in the last quantum well closest to p-EBL.It shows that the hole concentration in the mesa sidewalls region of device B is lower than that of device A,while the hole concentration in the middle mesa region of device B is higher than that of device A.

Fig.4. (a) Numerically calculated electric field profiles for devices A and B with the p-GaN/p-Al0.25Ga0.75N/p-GaN. (b) Vertical hole concentration profiles in the MQW region and(c)lateral hole distribution in the last quantum well closest to the p-EBL for devices A and B.Data are calculated at the injection current density of 200 A/cm2.

It is worth noting that the secondary etched mesa for device B also contains surface defects and these are also considered in our physical model. Hence, it is necessary to extract the recombination current for devices A and B. Figures 5(a)and 5(b) show the calculated radiative recombination current density and SRH recombination current density for devices A and B, respectively. According to Fig. 5(a), we can find that the radiative recombination for device B is significantly higher than that for device A. Nevertheless, Fig. 5(b) demonstrates that the SRH recombination current density for device A becomes larger. Note, the inset of Fig. 5(a) presents the lateral radiative recombination rate in the last quantum well closest to p-EBL for devices A and B. We can see that neither of the two devices has strong radiative recombination rate at the defected mesa edge, while the radiative recombination rate in the central mesa region is higher for device B thanks to the enhanced hole injection efficiency therein. The inset of Fig. 5(b) demonstrates that the defected mesa regions have a significant SRH nonradiative recombination rate. However,the secondary etched mesa helps suppress the SRH nonradiative recombination rate at the mesa edge for device B when compared with device A.Therefore,with the assistance of our physical calculations, we further confirm that the p-GaN/p-Al0.25Ga0.75N/p-GaN structure can produce hot holes and favor the hole injection into the MQW region.In the meanwhile,the secondary etched mesa can effectively suppress the SRH nonradiative recombination at the defected mesa edges. We also find that the newly generated surface defects at the secondary etched mesa edge sacrifice neither the hole injection nor the optical power.

It is known that the surface defects at the mesa sidewalls provide current leakage channels. Thus, the current–voltage(I–V)characteristics for the two μLEDs are measured and investigated, which are shown in Fig.6. When the two μLEDs are reversed biased at the voltage of-5 V,the leakage current for device B is almost one order of magnitude smaller than that for device A. The on/off current ratios at the biases of-5 V and 5 V are 108and 109for devices A and B, respectively.The reduced leakage current and the increased on/off current ratio infer that device B can effectively suppress the surface nonradiative recombination and reduce the leakage current on the mesa sidewalls. We also find that the forward voltage for device B is reduced when compared with device A,and this is due to the hot holes and the enhanced hole injection efficiency.

Fig.5. (a)Radiative recombination current density and(b)SRH recombination current density as a function of injection current density for devices A and B.The insets in(a)and(b)show the lateral radiative recombination rate and the lateral SRH nonradiative recombination rate in the last quantum well closest to the p-EBL layer,respectively.

Fig.6. Measured I–V characteristics in semi-log scale for devices A and B,respectively.

4. Conclusion

The secondary etched mesa and p-GaN/p-Al0.25Ga0.75N/p-GaN structure are proposed and the detailed analysis has been conducted for GaN-based μLEDs in this work. By using the p-GaN/p-Al0.25Ga0.75N/p-GaN structure,the polarization induced electric field therein can increase the kinetic energy for holes and hence the holes are more efficiently injected into the MQWs. For that reason, the EQE is increased by 155.6% at the current density of 200 A/cm2and the efficiency droop is suppressed to 43.8% for the proposed μLED.Meanwhile,the secondary etched mesa can also suppress the hole diffusion towards the mesa sidewalls and confine the holes into the central mesa region. Correspondingly, the surface SRH nonradiative recombination and the leakage current can be obtained and a high on/off current ratio of 109can be generated for the proposed μLED.Therefore,we strongly believe that the findings in this work are very helpful for the community to better understand GaN-based μLEDs and the proposed structure paves a new way for making highefficiency and strong-reliability GaN-based μLEDs.

Acknowledgments

This work was supported in part by the National Natural Science Foundation of China (Grant Nos. 62074050 and 61975051); Research Fund by State Key Laboratory of Reliability and Intelligence of Electrical Equipment,Hebei University of Technology(Grant Nos.EERI PI2020008 and EERIPD2021012); and Joint Research Project for Tunghsu Group and Hebei University of Technology (Grant No.HI1909).

主站蜘蛛池模板: 无码 在线 在线| 中文字幕亚洲综久久2021| 伊人久热这里只有精品视频99| 亚洲一级毛片在线播放| 国产精品嫩草影院视频| 老司机午夜精品网站在线观看| 黄色片中文字幕| 亚洲系列中文字幕一区二区| 中文字幕欧美成人免费| 在线观看国产精美视频| 久久精品免费国产大片| 成年免费在线观看| 久久久久青草线综合超碰| 欧美日本二区| 久久久久中文字幕精品视频| 手机精品福利在线观看| 强奷白丝美女在线观看| 日韩精品欧美国产在线| 国产自产视频一区二区三区| 亚洲一区二区三区中文字幕5566| 国产欧美日韩一区二区视频在线| 性色一区| 亚洲精品无码久久久久苍井空| 在线免费a视频| 成人免费一级片| 亚洲第七页| 国内精品伊人久久久久7777人| 99热国产在线精品99| 2021国产精品自产拍在线| 日韩欧美国产成人| 欧美精品一区在线看| 黄色a一级视频| 日本午夜影院| 首页亚洲国产丝袜长腿综合| 91精品啪在线观看国产91| 天堂在线亚洲| 欧美日韩国产高清一区二区三区| 露脸真实国语乱在线观看| 国产成人一二三| 免费在线一区| 久久综合成人| 欧美日本在线播放| 国产视频一区二区在线观看| 呦视频在线一区二区三区| 免费国产不卡午夜福在线观看| 亚洲IV视频免费在线光看| 国产欧美成人不卡视频| 亚洲香蕉在线| 午夜一区二区三区| 亚洲人成网站色7777| 成人国产一区二区三区| 刘亦菲一区二区在线观看| 又爽又大又光又色的午夜视频| 在线观看欧美国产| 四虎影视库国产精品一区| 亚洲美女高潮久久久久久久| 欧日韩在线不卡视频| 国产一区二区三区日韩精品| 亚洲精品少妇熟女| 亚洲AV无码乱码在线观看裸奔| 亚洲日韩精品伊甸| 国产一区二区三区精品欧美日韩| 华人在线亚洲欧美精品| 欧美人在线一区二区三区| 99视频精品在线观看| 秋霞一区二区三区| 54pao国产成人免费视频| 国产黄色免费看| 久久久亚洲色| 亚洲欧美另类专区| 亚洲人成网7777777国产| 一本久道久久综合多人| 高清精品美女在线播放| 99久久精品国产综合婷婷| 国产精品大白天新婚身材| 欧美综合中文字幕久久| 茄子视频毛片免费观看| 中文字幕人妻无码系列第三区| 欧美不卡在线视频| 亚洲va欧美ⅴa国产va影院| 国产在线无码一区二区三区| 国产一区二区三区夜色|