999精品在线视频,手机成人午夜在线视频,久久不卡国产精品无码,中日无码在线观看,成人av手机在线观看,日韩精品亚洲一区中文字幕,亚洲av无码人妻,四虎国产在线观看 ?

Influence of salt fog test on the performance of the composite coating on avionics cases

2014-03-18 07:19:26ChengyuJUXiaohuiWANGRunZHUXiaomingREN
機(jī)床與液壓 2014年6期

Cheng-yu JU,Xiao-hui WANG,Run ZHU,Xiao-ming REN

Reliability and Systems Engineering,Beihang University,Beijing 100191,China

1.Introduction

Metal/coating system is widely used to protect substrate material from corroding and improve service life by the aircraft and other weapons and equipment[1 - 2],the contribution of the coating includes shielding effect,resistance effect,cathodic protection,and so on[3 -4].These effects mainly depend on the film-forming materials of the coating and inhibiting pigment.The coating on the avionics cases can be corroded by the salt fog environment in ocean areas over time.At last the coating ages and then falls off[5].What’s more,lots of heat is generated by the computer inside the avionics cases,it leads to the coating in a high temperature environment.The corrosion and damage of the coating is largely accelerated by the salt fog and the high temperature.Metal/coating system during the process of failures always accompanies a series of electrochemical changes[6 -7].The information about metal corrosion and protective properties of organic coatings can be available through detecting changes of electrochemical signals[8 -12].In this paper,the properties of composite coating in high temperature and salt fog environment were studied through the Electrochemical Impedance Spectroscopy(EIS),Infrared Spectroscopy(IR)and Scanning Electron Microscopy(SEM).

2.Test methods and test scheme

2.1.Test material

The metal substrates of sample were 2A12 aluminum which is widely used as the aircraft materials,the topcoat material of the composite coating was polyurethane enamel,and the prime material was yellow zine acrylic polyurethane varnish.

2.2.Test conditions

The composite coating on the avionics cases is protected from ultraviolet radiation inside the aircraft,but it works in the coastal areas and can be destroyed by the salt fog and high temperature.So the salt fog test was scheduled to examine the performance of the coating.

NQ-1000A? salt spray cabinet was used in the laboratory test.Test conditions,according to MILSTD-810[13],were as follows:the NaCl concentration was 5% with a PH value of ~6.5 ~7.2,the temperature was 50℃± 1℃,and the fall out rate was 1.5 mL/80(cm2·h).

2.3.Measurement of EIS

Potentiostat/Galvanos-tat Model 263A? potentiostatic instrument and PAR M5210 ? lock-in amplifier were used for the information of the EIS in the laboratory test.Sample area tested by the EIS was 0.785 cm2,test solution was 5% NaCl solution,the traditional three-electrode system was performed,reference electrodes were calomel electrode,and auxiliary ones were platinum electrode.The spectrum was obtained with zero DC offset using frequency range of 10-2~105Hz and AC amplitude of 20 mV.

3.Results and discussion

3.1.EIS and modeling

Results of the EIS measurements in the form of bode and nyquist plots are shown in Figure 1 and Figure 2.Z indicates the electrochemical impedance,and F indicates the frequency.From these Figures 1~2,it can be seen that the value of the low frequency impedance is very high and almost reach to 1 010 Ω·cm2,it means the coating is similar to a pure capacitor,fewer defects of the coating exist before the salt fog test.The coating can protect the metal substrate against corrosion because that the salt ions can be blocked.The EIS spectra from attached films were analyzed using nonlinear least squares fitting(with ZSimWin)to an R[QR]model circuit as illustrated in Figure 3.Rs indicates solution resistance.Qc and Rc indicate coating capacitor and its resistor.The value of coating capacitor and its resistor are 6.461 ×10-10F and 1.1 ×1010Ω respectively according to the analysis on equivalent circuit.

The water molecules penetrate through the pore of coatings and finally reach to the metal interface as the time goes.Electric double layer capacitor which was connected in parallel with the interfacial resistance would be produced on the corrosion interface,and then causes the corrosion reaction.Because the corrosion process took place in the bottom of coatings,there are series systems between the hole resistance and the interfacial reaction of resistance.

Figure 1.Nyquist plot for coating before the salt fog test

Figure 2.Bode plot for coating before the salt fog test

Figure 3.Model circuit for coating before the salt fog test

There are few holes and defects in the bottom to be penetrated by the water molecules at the early reaction period.The barrier is still existence for the coating.The coating capacitance(Qc)and pore resistance(Qc//Rt)compose parallel system.

Results of the EIS measurements in the form of nyquist plots and R[Q[R[QR]]]model circuit after 345 hours exposure are shown in Figure 4 and Figure 5.The value of coating resistor is 1.65 ×109Ω according to analysis on equivalent circuit.

Soon afterwards,weber impedance is emerged after long time corrosion(Figure 6).According to the result of SEM,it can be judged that the existent of the pigment of zinc chrome yellow indicates that it is first corroded to protect the metallic substrate.The product after chemical reaction attaches to the potential corrosion activity points and covers it.It is the reason of the emergence of weber impedance.The EIS spectra are analyzed using nonlinear least squares fitting(with ZSimWin)to an R[Q[R[Q[RW]]]]model circuit as illustrated in Figure 7.Zw indicates the weber impedance,and coating capacitor is taken place of phase components(Q)generally in this picture.Phase components(Q)is defined as follow:

Z(jω)=(Y0)-1(jω)-n

Y0indicates the constant,j indicates the imaginary unit,andω indicates the angular frequency.Obviously,phase components(Q)is ideal capacitors when n=1.

Figure 4.Nyquist plot for coating after 345 h exposure

Figure 5.Model circuit for coating after 345 h exposure

Figure 6.Bode plot for coating after 533 h exposure

Figure 7.Model circuit for coating after 533 h exposure

3.2.The analysis of the infrared spectrum

Infrared spectrum of the coating after the different exposure time is shown in Figure 8.Different functional groups can be analyzed.2 850 ~2 920 cm-1is CH2-dissymmetric stretching,The indicative peak of C =O stretching vibration appears at 1 728 cm-1and 1 688 cm-1,The peak near 1 515 cm-1is C-N- stretching vibration from polyurethane.The peak of CH2-symmetrical bending and CH3-unsymmetrical bending appears at 1 450 cm-1.

Figure 8.Infrared spectrum after different exposure time

It can be found that peak positions and peak height do not change according to the result of infrared spectroscopy(IR).It means that the elemental composition of the coating does not change during the experiment.So,physical factor is the main reason for the coating damage rather than chemical factor.

3.3.Morphology by scanning electron microscope

The change of coating morphology is shown in Figure 9 and Figure 10.It can be seen that the adhesive is gradually eroded away after the salt fog test.

Only hard particles phase is left,there are some small holes and other defects on the surface of the coating.It is the source that pitting corrosion occurs on the metal.What is more,the integrity is affected by the micro defect.The main reason for the coating failure is that the electrolyte penetrates into the coating through micro-holes and defects,finally reaches to the metal substrate and causes corrosion on the metal.The corrosion products which are generated by the chemical reaction block the micro-holes and defects and reduce the permeability of oxygen.

As presented in Figure 11,cathode and anode region are separated because the higher oxygen permeates in other parts.There is a lower PH value in the anode region,but higher PH value in the cathode region.Corrosion products are generated as the diffusion of the anions and cationic.Blister or peeling happens with the increase of the corrosion products.It expands the contact area between the metal substrate with liquid electrolyte.This will result in the worse corrosion generally.

Figure 9.Coating morphology before the salt fog test

Figure 11.Schematic diagram of electrochemical corrosion

4.Conclusion

1)The degradation process of the coating can be accurately characterized by EIS which not only characterizes the corrosion mechanism according to the process of corrosion but also quantitatively studies the degradation process of resistor and capacitor.There will be a better result with the help of EIS and IR.The salt fogs play a very important effect on coating failures.

2)The content and types of the functional groups have not changed according to the IR after the salt fog test.The most likely reason is that the salt fogs have a strong corrosive.After a long period,the coating is eroded.The water molecules reach to the metallic substrate by micro-holes and defects.At last the metal substrate is corroded quickly,and then bubble and crack also happen.

[1]Zhou C,Lu X,Xin Z,et al.Hydrophobic benzoxazinecured epoxy coatings for corrosion protection[J].Progress in Organic Coatings,2013,76(9):1178-1183.

[2]Song Enpeng,Liu Wenting,Yang Xu.Study on accelerated corrosion test environment spectrum for internal aircraft structure[J].Acta Aeronautica et Astronautica Sinica,2006,27(4):643-649.

[3]Ranjbar,Z,Moradian S,Attar M R M Z.EIS investigation of cataphoretically electrodeposited epoxy coatings having different EEWs[J].Progress in organic coatings,2004,51(2):87-90.

[4]Le Pen C,Lacabanne C,Pébère N.Characterisation of water-based coatings by electrochemical impedance spectroscopy[J].Progress in organic coatings,2003,46(2):77-83.

[5]Luo Zhenhua,Yao Pei,Cai Jianping,et al.Progress ofevaluation techniques for organic coatings performance[J].Corrosion Science and Protection Technology,2004,16(5):314-317.

[6]Hinderliter B R,Croll S G,Tallman D E,et al.Interpretation of EIS data from accelerated exposure of coated metals based on modeling of coating physical properties[J].Elctrochimica Acta,2006,51(21): 4505-4515.

[7]Zhang Jintao,Hu Jiming,Zhang Jianqing,et al.A review on modern method of organic coatings[J].Journal of Materials Science and Engineering,2003,21(5): 763-768.

[8]Darowicki K,Slepski P,Szocinski M.Application of the dynamic EIS to investigation of transport within organic coatings[J].Progress in Organic Coatings,2005,52(4):306-310.

[9]Bierwagen G,Tallman D,He J P,et al.EIS studies of coated metals in accelerated exposure[J].Progress in Organic Coatings,2003,46(2): 148-157.

[10]Sharer Z,Sykes J.Insights into protection mechanisms of organic coatings from thermal testing with EIS[J].Progress in Organic Coatings,2012,74(2):405-409.

[11]Fredj N,Cohendoz S,F(xiàn)eaugas X,er al.Ageing of marine coating in natural and artificial seawater under mechanical stresses[J].Progress in Organic Coatings,2012,74(2):391-399.

[12]ZHANG W,WANG J,LI Y N,et al.Evaluation of metal corrosion under defective coatings by WBE and EIS technique[J].Acta Physico-Chimica Sinica,2010,26(11):2941-2950.

[13]Zuo S,Yao C,Liu W,et al.Porous palygorskite-polythiophene conductive composites for acrylic coatings[J].Journal of Applied Polymer Science,2013,129(5):2707-2715.

[14]MIL-STD-810 Committee.Environmental Test Methods and Engineering Guides[S].MIL-STD-810F,2000.

主站蜘蛛池模板: 国产日本视频91| 欧美成人精品一级在线观看| 97se亚洲| 午夜日b视频| 欧美国产精品不卡在线观看| 精品無碼一區在線觀看 | 亚洲成人一区在线| 日韩中文精品亚洲第三区| 久久免费成人| 国产玖玖视频| 狠狠亚洲婷婷综合色香| 欧美国产综合色视频| 日韩精品中文字幕一区三区| 日本欧美精品| 色欲色欲久久综合网| 日本精品αv中文字幕| 免费在线色| 亚洲中文字幕无码mv| 日韩小视频在线播放| 夜夜爽免费视频| AV熟女乱| 九色在线视频导航91| 精品福利视频导航| 亚洲欧美日韩动漫| 好久久免费视频高清| 成人亚洲国产| 国产微拍一区二区三区四区| 国产黄在线观看| 久久五月天国产自| 久久久久亚洲av成人网人人软件| 日本高清免费一本在线观看| 54pao国产成人免费视频| 国产成人免费高清AⅤ| 尤物亚洲最大AV无码网站| 国产精品女同一区三区五区| 又粗又大又爽又紧免费视频| 欧美a在线| 日本人真淫视频一区二区三区| 99热这里都是国产精品| 午夜视频在线观看免费网站| 又爽又大又黄a级毛片在线视频 | 国产成人资源| 88av在线看| 亚洲精品无码日韩国产不卡| 亚欧美国产综合| 国产尹人香蕉综合在线电影| 手机在线免费不卡一区二| 国产成人调教在线视频| 亚洲国产成人久久精品软件 | 成人日韩欧美| 欧美日本不卡| av天堂最新版在线| 国产一区二区三区视频| 狠狠干欧美| 国产成人精品第一区二区| 国产成人精品视频一区视频二区| 国产国语一级毛片在线视频| 精品福利网| 亚洲一级毛片在线观播放| 高清乱码精品福利在线视频| 91亚洲视频下载| 亚洲AV无码乱码在线观看裸奔| 成人午夜视频网站| 久久精品电影| 爱爱影院18禁免费| 欧美性色综合网| 天天综合色天天综合网| 国产一级毛片yw| 亚洲国产中文精品va在线播放| 亚洲男人的天堂久久香蕉| 看看一级毛片| 97视频免费在线观看| 第一区免费在线观看| 在线免费看片a| 97精品伊人久久大香线蕉| 91福利免费| 喷潮白浆直流在线播放| 国产成人综合日韩精品无码不卡 | 色婷婷成人| 国产精品成人观看视频国产| 国产欧美日本在线观看| 久久一本精品久久久ー99|